Cases

Cases and customers: reviews of nine production-line issues

We do not write “the customer was very satisfied.” We describe what the problem looked like, how it was identified, and how it was ultimately addressed. The evaluation process is more useful as a reference than the conclusion.

  • 9 cases
  • Including the evaluation process
  • De-identified
  • Data available under NDA

Deep Dives Three in-depth reviews: how to identify, how to improve

These three entries cover the complete troubleshooting chain—the phenomenon, the basis for the judgment at the time, what was changed, and the resulting figures. Because site conditions differ, the conclusions may not be directly transferable, but the evaluation sequence can be used as a reference.

12-inch wafer fab · Post-CMP cleaning

Particle counts periodically rebound, although the brush rollers appear intact

Problem
Particle counts rebounded approximately every three weeks after cleaning; replacing the brush roller restored performance, and the site treated this as “the brush roller reached the end of its service life.”
Approach
A lower-extractable formulation was introduced, and baselines for pore unclogging and water absorption were established, changing the replacement criterion from a calendar-based cycle to data thresholds.
Results
Particle count decreased relative to the baseline 62%, and the service life of each roller was extended from 30 days to 52 days。
View the complete review
PCB manufacturer · Board surface cleaning

Static attraction causes residual debris to remain after dust removal

Problem
Fine debris remained attached to the board surface after dust removal, requiring manual rework before AOI and extending the takt time.
Approach
Switch to a two-step combination of a 10³–10⁶Ω conductive wire plate brush + a handheld antistatic toothbrush, and rectify the brush-body grounding path at the same time.
Results
Board surface debris defects decreased from 1.8% to 0.4%, and the rework station was reduced by 1 person per line.
View the complete review
Advanced packaging plant · IC carrier deburring

FC-BGA carrier edge burrs cause placement misalignment

Problem
The burr height along the cut edges of the carrier varied, resulting in intermittent placement misalignment during assembly.
Approach
Nylon 612 abrasive filaments + a spiral-wound structure, with the end chamfer customized to the board-edge profile and the compression calculated inversely from line speed.
Results
Stable burr height ≤ 25 μm, placement misalignment defects decreased 71%。
View the complete review

Case data were taken from customer acceptance records and are presented in de-identified form; test conditions and acceptance criteria can be provided together with factory audit documentation.

Field Notes Six additional site records

The following cases come from actual communications and on-site troubleshooting, with customer information de-identified. We describe “how the issue was identified” as clearly as possible because the evaluation process is more useful as a reference than the conclusion—your site conditions differ, so the conclusions may not be directly transferable, but the troubleshooting approach can be.

CMP · 12 inches

Regular arc-shaped scratches at the edge; replacing the brush roller only provides short-term improvement

Background
In the post-CMP cleaning section, regular arc-shaped scratches appeared within a 5 mm annular band at the wafer edge. Replacing the brush roller improved the condition temporarily, but the scratches reappeared within two weeks.
Evaluation
Disassembly revealed a sudden change in hardness at the brush roller end and mold flash on the end face; at the same time, shaft-end runout exceeded the recommended limit for that rotational speed. Contact pressure was concentrated at the end, forming a fixed arc.
Action
A transition treatment was applied to the end, with end-face flatness and runout controlled as separate items; compression was mandatorily retested after roller replacement.
Results
The scratches did not recur, and particle counts remained at the baseline.
Carrier · FC-BGA

Board warpage exceeds the standard after deburring, while residual burr roots remain

Background
After deburring the thin FC-BGA substrate, the warpage exceeded the specification, and cross-sectional inspection still showed burr roots.
Evaluation
A single-pass parameter was intended to satisfy both material removal and flatness: high pressure bent the board, while low pressure resulted in insufficient removal. In addition, without backside support, the thin board underwent elastic deformation under pressure.
Action
The process was changed to two passes: rough deburring (larger compression) followed by fine finishing (finer grit and low pressure), with backside support added.
Results
Board warpage returned to within specification, and the burr roots were eliminated.
Equipment Maintenance · Chamber

Particle counts increased after maintenance

Background
After the equipment chamber was maintained according to procedure, particle counts rose over three consecutive batches, with no changes to process parameters.
Evaluation
Short segments of brush filament debris were found inside the chamber. The source was the unsealed end of the strip brush—the cut end was continuously shedding short filaments.
Action
The strip brush ends were changed to an adhesive-sealing treatment, and a dedicated maintenance tool was introduced, with an inventory count performed before and after maintenance.
Results
Particle counts returned to baseline, and no recurrence of the issue was observed.
Front End · 8-inch

Particle counts increased after installing a new brush roller

Background
After the front-end brush-washing section was changed to a new brush roller, the particle removal rate decreased. The brush roller showed no visible differences from a new roller.
Evaluation
Three factors overlapped: residual material on the end face of the new roller had not been pre-cleaned, the cleaning fluid had not been replaced simultaneously, and the new roller's outside-diameter tolerance resulted in excessive compression.
Action
A pre-cleaning step was added before bringing the new roller online; compression was mandatorily retested after roller replacement; and the cleaning fluid replacement cycle was decoupled from brush roller replacement.
Results
Particle counts recovered and remained stable within the baseline range.
PCB · Surface Dust Removal

Dust returned after cleaning

Background
After dust removal from the PCB surface, particles were still found during sampling, concentrated in the same area.
Evaluation
Static electricity generated by friction from the conventional nylon roller brush caused dust to be re-adhered; grounding at the shaft end in this area was inadequate, preventing charge dissipation.
Action
A conductive filament roller brush was adopted, the shaft-end grounding path was repaired, and it was included in periodic ESD testing.
Results
Surface cleanliness met the requirements, and grounding resistance was within the controlled range.
Quartz · Furnace tube

Longitudinal scratches on the inner wall, aligned with the travel direction

Background
Longitudinal scratches appeared on the inner wall of the quartz tube after cleaning, in the same direction as the brush travel direction.
Evaluation
Metal was exposed at the brush joint, and the long handle lacked sufficient straightness, causing the brush head to deflect to one side during travel and creating uneven pressure.
Action
The joint was changed to a fully encapsulated design with a smooth transition; the long handle was sectioned, with intermediate guides added.
Results
The scratches no longer appeared, and cleaning efficiency improved at the same time.

Quantitative data (particle counts, warpage, and service-life comparisons) are available within the scope of the confidentiality agreement.

Trusted by Manufacturers we have served over the long term

The following are some of the customer identifiers used to illustrate the scope of industry coverage. The identifiers belong to their respective rights holders and do not imply endorsement or authorization.

CRRC
KONE
Mitsubishi
Otis
Combi
Fangda

How we work Beyond the cases, how we usually collaborate

  • Start with on-site data

    Particle counts, scratch morphology, replacement records—data is much faster than descriptions. If you do not have data, we will tell you what to record.

  • Offer 2–3 options, not just one.

    The trade-offs differ by solution: cost, service life, and risk. You decide which is more appropriate, rather than having us decide for you.

  • Sample validation

    Sample lead times are confirmed according to the drawings, with material and batch identifiers included. We recommend running them first on non-critical batches.

  • Lock in the parameters before discussing volume production

    After the samples pass, document the compression, rotational speed, and acceptance method to prevent performance drift after changing batches.

  • Customer requirements

    Leave your contact details and requirements so we can get in touch.

    Operating conditions and dimensions

    Optional. Saved details are included with your inquiry.